        有色差

        There is a color difference

        產生原因石膏粉

        Cause of occurrence

        1、膩子粉本身屬于半成品,原材料不穩定是導致色差的主要原因之一,由于礦區開采出來的礦粉會因區域不同而品質不同,如未注意調配,就會出現各個批次不同而色差。

        1. Putty powder itself is a semi-finished product, and the instability of raw materials is one of the main reasons for color difference. Due to the different quality of mineral powder extracted from mining areas, if not properly mixed, color difference may occur in different batches.

        2、由于有些廠家使用“濫竽充數”的方法將低等級原料混雜發貨,因為采購的數量較大,無法逐一抽檢到位,導致有個別“漏網之魚”參雜在生產里面導致個別性的色差。

        2. Due to some manufacturers using the method of "filling numbers with inferior materials" to mix and ship low-grade materials, the large quantity purchased cannot be inspected one by one, resulting in individual "missed fish" mixed in production and causing individual color differences.

        3、由于生產人員失誤將不同等級的原料參雜在一起生產引起的色差或將不同品牌的產品批刮在同一面墻上而引起的色差。

        3. Color difference caused by production personnel mistakenly mixing different grades of raw materials together or scraping different brands of products on the same wall.

        處理方法

        processing method

        1、色差一般不是配方問題,所以不存在質量問題,如要上漆的墻面一般是可以用漆膜遮蓋過去,不會影響整體裝飾效果,如一般批刮二、三道不上漆的墻面出現色差,建議其再批刮一道無色差的膩子粉或上漆。

        1. Color difference is generally not a formula issue, so there is no quality problem. For walls that need to be painted, they can generally be covered with paint film without affecting the overall decorative effect. If color difference occurs when scraping two or three layers of unpainted walls, it is recommended to scrape another layer of colorless putty or paint.

        2、所有參與生產及施工的人員應嚴格按照有關標準進行生產和施工,避免產生人為的質量問題。

        2. All personnel involved in production and construction should strictly follow relevant standards to avoid human caused quality problems.

        脫粉

        De powdering

        產生原因

        Cause of occurrence

        1.施工原因:由于油漆師傅在最后一道收光施工時多次用刮刀干刮墻面而引起的表面細微的起皮現象,等干燥后就會形成脫粉癥狀。

        1. Construction reason: Due to the painter's repeated use of a scraper to dry scrape the wall surface during the final finishing process, there is a slight peeling phenomenon on the surface, which will cause powdering symptoms after drying.

        2.人為原因:由于最后一道施工膩子未干時,遇到外來粉塵附著到墻面上(切割作業,大風,清理地板等)導致的墻面假象脫粉。

        2. Human factors: Due to the last layer of construction putty not drying yet, external dust adhered to the wall surface (cutting operations, strong winds, cleaning floors, etc.), causing the wall surface to appear powdery.

        3.生產原因:由于生產人員粗心將原料配方比例放錯,或因機臺設備卸漏,導致的配方不穩定而引起的脫粉。

        3. Production reasons: Powder shedding caused by unstable formula due to careless placement of raw material formula ratios by production personnel or leakage of machine equipment.

        處理方法

        processing method

        1.施工師傅在做最后一道不上漆收光施工時應注意膩子的表面濕度,太干時會引起起皮脫粉,在收光時將刀痕修平即可,不宜多次干刮。

        1. The construction master should pay attention to the surface humidity of the putty when doing the last unpainted finishing construction. If it is too dry, it will cause peeling and powdering. When finishing, the knife mark can be smoothed out, and it is not advisable to dry scrape it multiple times.

        2.如出現粉塵附著在墻面上造成的假象脫粉的應待裝修完畢后用雞毛彈清除粉塵,或用清水與干凈的布條擦拭干凈即可。

        If dust adheres to the wall and causes false detachment, it should be removed with a chicken feather ball after decoration is completed, or wiped clean with water and a clean cloth strip.

        3.如出現快干脫粉的,應等公司技術人員到現場鑒定是否是由于產品配方引起的原因。

        3. If there is fast drying and powdering, the company's technical personnel should wait on site to identify whether it is caused by the product formula.

        本文由 濟南膩子粉 友情奉獻.更多有關的知識請點擊  http://www.daquanq.com.cn   真誠的態度.為您提供為全面的服務.更多有關的知識我們將會陸續向大家奉獻.敬請期待.

        This article is a friendly contribution from Jinan Putty Powder For more related knowledge, please click http://www.daquanq.com.cn Sincere attitude To provide you with comprehensive services We will gradually contribute more relevant knowledge to everyone Coming soon.

      ??? 主站蜘蛛池模板: 亚洲欧美中文v日韩v在线| 在线观看国产精品自拍| 青青草亚洲在线一区观看| 国产精品久久久久久一区二区三区 | 国产精品美女AV免费观看| 亚洲天天影院色香欲综合| 精品日韩卡1二2卡3卡4卡乱码| 国内免费av在线播放| 好紧好爽好深再快点av在线| 亚洲一区二区三区无吗| 天天澡天天揉揉AV无码人妻斩| 国产一区二区牛影视| 伊人狠狠色j香婷婷综合| 内射干少妇亚洲69XXX| 青青草免费观看高清视频| 国产精一品亚洲二区在线播放| 国产一区二区三区视频免费| 彩票| 国产成人久久精品77777综合| 免费中文字幕无码视频| 国产免费无遮挡吸乳视频| 亚洲AV无码成人精品区H| 婷婷激情五月综合在线观看| 国产av一区二区3区| 69av视频在线| 老司机午夜精品视频无码| 99久久精品国产一区二区暴力 | 亚洲福利第一页在线观看| 国产亚洲欧洲aⅴ综合一区| 久久人妻视频免费观看| 亚洲精品亚洲人成在线下载| 初尝人妻少妇中文字幕在线| 国产一级黄色片在线观看| 亚洲精品久久久蜜桃一区| 精品久久久久88久久久| 国产精品流白浆喷水| 亚洲男人综合久久综合天堂| 日韩av在线不卡一区二区三区| 亚洲国产精品国自产电影| 亚洲色欲色欱WWW在线| 欧美成人一区二区三区不卡|